| Order | Test Name | Result | Exam Conditions | |
|---|---|---|---|---|
| 1 | State Physical Properties |
Hardness(HS) | 54 | 170℃×10min 2nd Vulcanization 150℃×2Hr |
| Tensile Strength(Kg/㎠) | 203 | |||
| Elongation Rate(%) | 641 | |||
| 2 | Heat Resistance Test |
Hardness Change Rate(HS) | 3 | 120℃×70hrs |
| Tensile Strength Change Rate(Kg/㎠) | 9.9% | |||
| Elongation Rate Change(%) | -13.9% | |||
| 3 | Compression Permanent Shrinkage Rate(%) | 26.2% | 120℃×70hrs Production 170℃ * 40min 2nd Vulcanization 150℃×2Hr |
|