| Order | Test Name | Result | Exam Conditions | |
|---|---|---|---|---|
| 1 | State Physical Properties | Hardness(HS) | 70 | 170℃×10min 2nd Vulcanization 150℃×2Hr |
| Tensile Strength(Kg/㎠) | 162 | |||
| Elongation Rate(%) | 342 | |||
| 2 | Heat Resistance Test |
Hardness Change Rate(HS) | 4 | 150℃×70hrs |
| Tensile Strength Change Rate(Kg/㎠) | -6.8% | |||
| Elongation Rate Change(%) | 8.8% | |||
| 3 | Compression Permanent Shrinkage Rate(%) | 10.6% | 150℃×70hrs Production 170℃ * 40min 2nd Vulcanization 150℃×2Hr |
|
| 12% | 150℃×70hrs Production 180℃ * 15min |
|||
| 11.3% | 150℃×70hrs Production 180℃ * 15min 2nd Vulcanization 150℃×4Hr |
|||