| Order | Test Name | Result | Exam Conditions | |
|---|---|---|---|---|
| 1 | State Physical Properties |
Hardness(HS) | 72 | 170℃×15min Post Cure 175℃ x 4Hr |
| Tensile Strength(Kg/㎠) | 81.095 | |||
| Elongation Rate(%) | 130.1 | |||
| 2 | Heat Resistance Test |
Hardness Change Rate(HS) | 6 | 150℃×70hrs |
| Tensile Strength Change Rate(Kg/㎠) | 10.6% | |||
| Elongation Rate Change(%) | -4.92% | |||
| 3 | Oil Resistance Test |
Hardness Change Rate(HS) | 3 | 150℃×70hrs NO1 |
| Tensile Strength Change Rate(Kg/㎠) | 4.3% | |||
| Elongation Rate Change(%) | 3.07% | |||
| Volume Change Rate(%) | -4.23% | |||
| Hardness Change Rate(HS) | -13 | 150℃×70hrs NO3 |
||
| Tensile Strength Change Rate(Kg/㎠) | -10.8% | |||
| Elongation Rate Change(%) | -1.23% | |||
| Volume Change Rate(%) | 11.14% | |||
| 4 | Compression Permanent Shrinkage Rate(%) | 15% | 150℃×70hrs | |
| 5 | Ozone Resistance Test | NO CRACK | 50ppm x 40℃x 8Hr x 5% Elongation | |
| 6 | Low Temperature Elastic Recovery Test(TR10) | -45℃ | KTR Test Request | |