| Order | Test Name | Result | Exam Conditions | |
|---|---|---|---|---|
| 1 | State Physical Properties |
Hardness(HS) | 63 | 170℃×10min 2nd Vulcanization 150℃×2Hr |
| Tensile Strength(Kg/㎠) | 111 | |||
| Elongation Rate(%) | 279 | |||
| 2 | Heat Resistance Test |
Hardness Change Rate(HS) | 3 | 120℃×168hrs Specimen Preparation Methods 170℃×10min 2nd Vulcanization 150℃×2Hr |
| Tensile Strength Change Rate(Kg/㎠) | -5.4% | |||
| Elongation Rate Change(%) | -11.1% | |||
| 3 | Oil Resistance Test |
Hardness Change Rate(%) | -1 | 100℃×70hrs Antifreeze(coolant) Concentrate MS 591-14 |
| Tensile Strength Change Rate(Kg/㎠) | -17.1% | |||
| 4 | Compression Permanent Shrinkage Rate(%) | 6.2% | 95℃×168hrs Specimen Preparation Methods 170℃×40min |
|
| 5 | Low Temperature Recovery Test(TR10) | -46.7℃ | Lysault Request | |