| Order | Test Name | Result | Exam Conditions | |
|---|---|---|---|---|
| 1 | State Physical Properties |
Hardness(HS) | 63 | 170℃×6min |
| Tensile Strength(Kg/㎠) | 133 | |||
| Elongation Rate(%) | 539 | |||
| 2 | Heat Resistance Test |
Hardness Change Rate(HS) | 5 | 100℃×70hrs |
| Tensile Strength Change Rate(Kg/㎠) | 23.3% | |||
| Elongation Rate Change(%) | 39.7% | |||
| 3 | Oil Resistance Test |
Hardness Change Rate(HS) | 4 | 100℃×70hrs NO1 |
| Tensile Strength Change Rate(Kg/㎠) | 0.8% | |||
| Elongation Rate Change(%) | 28.9% | |||
| Modulus of Volume Change(%) | -1.2% | |||
| Hardness Change Rate(HS) | -6 | 100℃×70hrs NO3 |
||
| Tensile Strength Change Rate(Kg/㎠) | -33.1% | |||
| Elongation Rate Change(%) | -44.1% | |||
| Modulus of Volume Change(%) | 16.6% | |||
| Hardness Change Rate(HS) | 0 | 100℃×70hrs WATER |
||
| Modulus of Volume Change(%) | 0.1% | |||
| 4 | Compression Permanent Shrinkage Rate(%) | 19.5% | 100℃×70hrs Production 170℃ * 40min |
|